Key takeaways
- Most filaments are hygroscopic, meaning they absorb water from the air; nylon, TPU, PC and PVA absorb the most.
- Wet filament pops and bubbles in the nozzle, strings more and prints rough, weaker parts.
- Makers suggest drying PLA at about 45 to 55°C for 6 to 8 hours, and nylon, PC and TPU hotter or longer.
- A dedicated filament dryer is the safest method; Prusa and Elegoo warn against kitchen ovens, whose temperature control is imprecise.
Drying 3D printer filament means gently heating a spool for several hours to drive out the moisture it has absorbed from the air. This guide explains why filament gets wet, how to spot it, the temperatures and times to use for 8 materials, 4 ways to dry it, and how to store it dry.
Why does 3D printer filament get wet?
Most filaments are hygroscopic: they absorb water from the air, and more humidity and time mean more absorption, says Prusa. In the hot nozzle, that water turns to steam, which makes extrusion unstable and leaves voids in the plastic, according to Bambu Lab and Elegoo.
Some materials absorb far more than others. MatterHackers gives these typical moisture levels for 5 materials:
| Filament | Moisture it can absorb |
|---|---|
| Nylon (PA6) | About 2.5 to 9.5% |
| TPU | About 0.3 to 3% |
| PETG | About 0.5 to 2% |
| PLA | About 0.3 to 1% |
| ABS and ASA | About 0.2 to 0.8% |
PVA, the support material, dissolves in water. Prusa says PLA changes little with moisture, while nylon is affected significantly.
What are the signs of wet filament?
Popping or hissing at the nozzle is the clearest sign. Bambu Lab, MatterHackers and Prusa list these 6 symptoms:
- Popping, crackling or sizzling sounds while printing.
- Bubbles or steam as the filament extrudes.
- More stringing between parts.
- Rough or pitted surfaces, often the first sign, says Prusa.
- Weaker layer adhesion, so parts break more easily.
- Clogs or feeding problems in severe cases.
UltiMaker adds 2 material-specific clues: wet PVA turns soft and sticky, and clear nylon turns cloudy. MatterHackers notes that other faults cause some of these symptoms too, so drying a spool is a good first test.
What temperature and time should you dry filament at?
Most makers suggest 4 to 12 hours, at a temperature that depends on the material. Settings differ between makers, so follow the label on your spool first. These are Bambu Lab's oven settings and Prusa's settings for its own filaments:
| Filament | Bambu Lab | Prusa |
|---|---|---|
| PLA | 50°C, 8 hours | 45°C, 6 hours |
| PETG | 60 to 65°C, 8 hours | 55°C, 6 hours |
| ASA | 75 to 85°C, 8 hours | 80°C, 4 hours |
| TPU | 70°C, 8 hours | 60°C, 4 to 6 hours |
| PC | 75 to 85°C, 8 hours | 85°C, 5 hours (PC Blend) |
Don't go hotter than recommended. Prusa says too much heat softens filament so the strands stick together, and spools have limits too: Bambu rates its low-temperature spools to 70°C and UltiMaker says its spool can soften around 80°C.
How do you dry filament?
Use a dedicated filament dryer if you can; other methods work with care. These are the 4 main options:
- Filament dryer. Prusa recommends these, and many feed filament through a tube so you can print while it dries. Check that yours reaches your filament's temperature: Sunlu's S2 goes up to 70°C, and its E2 up to 110°C for engineering filaments.
- Food dehydrator. Prusa says to remove the trays and put the spool inside, but notes dehydrators usually only reach low temperatures.
- Printer heatbed. Bambu Lab documents this for its enclosed printers only, with the spool under a cover; flip it every 6 hours.
- Kitchen oven, as a last resort. Prusa warns that imprecise oven control can damage filament, especially PLA, and Elegoo says never to use a kitchen or microwave oven.
Airflow matters as much as heat, says Polymaker, because moving air carries the moisture away. A sealed box with desiccant keeps dry filament dry, but MatterHackers and UltiMaker say it won't dry a wet spool.
How do you keep filament dry?
Seal it with desiccant as soon as it's dry. Bambu Lab says to let a dried spool cool for 5 to 10 minutes, then seal it straight away. Follow these 4 storage tips:
- Use an airtight container: a dry box, the original bag with a clip, or a vacuum bag, each with desiccant inside.
- Keep humidity low: Elegoo suggests below 30% relative humidity at 15 to 25°C, and UltiMaker says 10 to 30% suits most materials.
- Print sensitive spools from a dryer: Polymaker suggests running a dryer while you print nylon in a humid climate.
- Refresh the desiccant: indicator beads change colour when spent. Bambu says its silica gel can be dried in an oven at 80 to 90°C and reused 5 to 15 times.
Dry filament makes a cleaner first layer, so pair this with our guide to 3D printer bed leveling. For ideas to print next, see our list of useful things to 3D print. Our Sunlu Kidoodle MiniBox A1 review tests Sunlu's kids' printer, and our 5 best 3D printers list compares current models.
Common questions
How long does it take to dry 3D printer filament?
Usually 4 to 12 hours, depending on the material. Prusa dries PLA for 6 hours at 45°C, Bambu Lab for 8 hours at 50°C, and Sunlu says nylon can take 8 to 24 hours or more.
Is 3 hours enough to dry PLA?
Usually not. None of the makers we checked suggest less than 4 hours: MatterHackers starts at 4 hours, Prusa and Elegoo say 6, and Bambu Lab and Creality say 8.
Is drying filament necessary?
For nylon, TPU, PC and PVA, yes: Bambu Lab and Creality mark drying as required. For PLA and PETG it's recommended when prints look wrong, and Bambu says sealed spools don't need frequent drying.
How do I keep 3D printer filament dry?
Seal it in an airtight box, its original bag or a vacuum bag with desiccant, and keep it below about 30% humidity in a cool, dark place, as Elegoo and UltiMaker suggest.